![](../../indexgifs/cructabswhthome.gif) |
|
|
REX M2®(S)
(AISI M2)
|
|
|
![](../prodbyappnavgifs/CrucDataHeader.gif) |
|
|
REX M2 is a tungsten-molybdenum high speed steel which gives outstanding performance in all operations where a general purpose high speed steel is required. REX M2 has a wide hardening range, excellent toughness, with good wear and red hardness characteristics. REX M2S is the sulfur-bearing counterpart of REX M2. The sulfur addition provides good grindability and an improvement in machinability of 25 to 35 per cent over a comparable nonsulfurized grade.
|
|
|
|
|
Typical Chemistry |
Carbon |
0.85% |
Manganese |
0.30% |
Silicon |
0.30% |
Chromium |
4.15% |
Vanadium |
1.95% |
Tungsten |
6.40% |
Molybdenum |
5.00% |
Sulfur |
0.03% max. (0.10%)
|
|
Typical Applications |
|
Broaches |
Milling Cutters |
|
Counterbores |
Punches |
|
End Mills |
Taps |
|
Form Tools |
Tool Bits |
|
|
|
|
|
|
|
|
|
|
- Annealed Hardness: 217/255 BHN
Machinability in the annealed condition is approximately 45% of W1 Tool Steel (1%C).
Thermal Treatments
Critical Temperature: 1530F(830C).
Forging: 2075F(1135C) Do not forge below 1700F(925C). Slow cool after forging.
Annealing: 1600F(870C), hold 2 hours, slow cool 25F(15C)/ hr max. to 1000F(535C), then air or furnace cool. Hardness BHN 217/255. Stress Relieving: 1100-1300F(595-740C), hold 2 hrs. and air or furnace cool.
Straightening: Best done warm 400-800F(205-425C.)
Hardening: (Salt Baths or Vacuum Furnace preferred.)
Preheat: 1500-1550F(815-845C), equalize.
High Heat: 2100-2225F(1150-1220C), soak 2 to 5 minutes. For vacuum hardening, use the high side of the high heat range and soak times.
Quench: Salt or oil to 1000-1100F(540-595C), equalize, then air cool to hand warm, 150F(65C). Temper immediately. The vacuum quench rate to below 1000F(540C) is critical to achieve comparable results.
Temper: Tempering at 1000F(540C) or higher 2 times for at least 2 hours at temperature is recommended. Air cool to room temperature between tempers.
|
|
|
|
|
|
Hardening Data
Oil quenched. |
|
Tempering
|
Hardness HRC
|
Temperature
|
2100F
(1150C)
|
2150F
(1175C)
|
2250F
(1230C)
|
°F
|
°C
|
|
975
|
524
|
64
|
65
|
66
|
1000
|
540
|
64
|
65.2
|
66.8
|
OPTIMUM FOR MAXIMUM TOUGHNESS AND EFFECTIVE STRESS-RELIEVING.
|
1025
|
550
|
63.5
|
65.1
|
66.8
|
1050
|
565
|
62.6
|
64.8
|
66
|
1075
|
580
|
61.3
|
64
|
65
|
1100
|
595
|
60
|
62.5
|
64
|
1125
|
605
|
58.4
|
60.5
|
62.4
|
1150
|
620
|
57
|
58
|
60.9
|
1175
|
635
|
|
|
59
|
1200
|
650
|
|
|
57
|
|
|
|
|
|
|
|
|
|
![](../../indexgifs/chemheatslug.gif) |
|
|
|
|
|
Size Change During Hardening |
|
- Hardening
- Temp.
|
- Tempering
- Temp.
|
HRC
|
- Longitudinal
- Size Change
%
|
°F
|
°C
|
°F
|
°C
|
|
2200
|
1204
|
1025
|
552
|
65
|
+.22
|
|
|
|
|
|
|
|
|
|
Surface Treatments
REX M2 can be nitrided, steam tempered or titanium-nitride coated if desired. If the CVD TiN treatment is used, care is required in vacuum hardening.
Physical Properties
Modulus of Elasticity ...................................................................30 psi x 106 (207 GPa)
Specific gravity ............................................................................................................8.14
Density .......................................................................................0.294 lb/in3 (8144 kg/m3)
Coefficient of Thermal Expansion
- Temperature
- Range
|
- Coefficient of Thermal
- Expansion
|
°F
|
°C
|
in/in/°Fx10-6
|
mm/mm/°Cx10-6
|
70- 500
|
21-260
|
6.40
|
11.5
|
70- 800
|
21-425
|
6.58
|
11.8
|
70-1000
|
21-540
|
6.72
|
12.1
|
|
|
|
|
|
|
|
|
Return to top of page
|
|
|
|
|
|